Ceramics (TiC with Ni additive), R0 =  5.280 g/cc

Target: 
  Sample density R0 = 5.28 g/cc, bulk sound velocity C0 = 7 km/s, longitudial sound velocity Cl = 9.15 km/s
  Sample thickness 10 mm 
Loading: 
  High explosive in contact with sample
Experiment type: Capacitor gauge

     t, mks     V, m/s

      0.000      0.000
      0.100     67.000
      0.200    188.000
      0.330    345.000
      0.400    390.000
      0.500    416.000
      0.600    421.000
      0.700    420.000
      0.800    418.000
      1.000    412.000
      1.200    407.000
      1.400    408.000
      1.600    408.000
      1.800    407.000
      2.000    407.000
      2.500    410.000
      2.880    410.000

References:
1. G. I. Kanel', A. A. Razorenov, A. V. Utkin, K. Baumung, Experimental profiles
   of shock waves, Preprint of Scientific Association IVTAN of RAS (1996)