Ceramics (TiC with Ni additive), R0 =  5.280 g/cc

Target: 
  Sample density R0 = 5.28 g/cc, bulk sound velocity C0 = 7 km/s, longitudial sound velocity Cl = 9.15 km/s
  Sample thickness 10 mm 
Loading: 
  Aluminum impactor 2 mm thick, impactor velocity 450 +/- 20 m/s
Experiment type: Capacitor gauge

     t, mks     V, m/s

      0.000      0.000
      0.100     97.000
      0.200    177.500
      0.260    200.000
      0.320    214.500
      0.370    220.000
      0.420    223.000
      0.470    224.000
      0.490    222.000
      0.600    194.000
      0.718    203.704
      0.780    205.000
      0.950    197.000
      1.200    201.000
      1.450    199.000
      1.950    199.000
      2.450    200.000

References:
1. G. I. Kanel', A. A. Razorenov, A. V. Utkin, K. Baumung, Experimental profiles
   of shock waves, Preprint of Scientific Association IVTAN of RAS (1996)