Ceramics (TiC with Ni additive), R0 =  5.280 g/cc

Target: 
  Sample density R0 = 5.28 g/cc, bulk sound velocity C0 = 7 km/s, longitudial sound velocity Cl = 9.15 km/s
  Sample thickness 11.9 mm 
Loading: 
  Aluminum impactor 7 mm thick, impactor velocity 1050 +/- 40 m/s
Experiment type: Capacitor gauge

     t, mks     V, m/s

      0.000      0.000
      0.060     27.000
      0.120     84.000
      0.200    189.000
      0.270    297.000
      0.339    383.915
      0.430    465.000
      0.540    507.000
      0.640    525.000
      0.760    531.000
      0.810    533.000
      0.850    535.000
      0.880    536.000
      0.990    533.000
      1.090    522.000
      1.170    535.000
      1.300    541.000
      1.410    546.000

References:
1. G. I. Kanel', A. A. Razorenov, A. V. Utkin, K. Baumung, Experimental profiles
   of shock waves, Preprint of Scientific Association IVTAN of RAS (1996)