Ceramics (TiC with Ni additive), R0 =  5.280 g/cc

Target: 
  Sample density R0 = 5.28 g/cc, bulk sound velocity C0 = 7 km/s, longitudial sound velocity Cl = 9.15 km/s
  Sample thickness 10 mm 
Loading: 
  Aluminum impactor 4 mm thick, impactor velocity 1500 +/- 50 m/s
Experiment type: Capacitor gauge

     t, mks     V, m/s

      0.000      0.000
      0.100    100.000
      0.200    300.000
      0.330    590.000
      0.405    695.238
      0.500    742.000
      0.600    758.000
      0.850    767.000
      0.950    755.000
      1.100    755.000
      1.500    766.000
      1.750    761.000

References:
1. G. I. Kanel', A. A. Razorenov, A. V. Utkin, K. Baumung, Experimental profiles
   of shock waves, Preprint of Scientific Association IVTAN of RAS (1996)