Ceramics (TiC with Ni additive), R0 =  5.280 g/cc

Target: 
  Sample density R0 = 5.28 g/cc, bulk sound velocity C0 = 7 km/s, longitudial sound velocity Cl = 9.15 km/s
  Sample thickness 12 mm 
Loading: 
  Aluminum impactor 4 mm thick, impactor velocity 1500 +/- 50 m/s
Experiment type: Capacitor gauge

     t, mks     V, m/s

      0.000      0.000
      0.070     19.000
      0.110     48.000
      0.170    110.000
      0.230    198.000
      0.270    263.000
      0.320    361.000
      0.380    476.000
      0.440    601.000
      0.490    669.000
      0.560    716.000
      0.640    733.000
      0.730    745.000
      0.820    756.000
      0.910    749.000
      0.980    738.000
      0.990    734.000

References:
1. G. I. Kanel', A. A. Razorenov, A. V. Utkin, K. Baumung, Experimental profiles
   of shock waves, Preprint of Scientific Association IVTAN of RAS (1996)