Copper M2, R0 =  8.930 g/cc

Target: 
  Sample density R0 = 8.93 g/cc, bulk sound velocity C0 = 3.96 km/s, longitudial sound velocity Cl = 4.6 km/s
  Sample thickness 3.9 mm (rod)
Loading: 
  Aluminum impactor 0.2 mm thick, impactor velocity 660 +/- 20 m/s
Experiment type: Capacitor gauge

     t, mks     V, m/s

      0.000      0.000
      0.020     11.000
      0.040     34.000
      0.050     62.000
      0.063    158.000
      0.070    194.000
      0.080    212.000
      0.090    205.000
      0.105    188.000
      0.135    145.000
      0.150    124.000
      0.179    136.596
      0.190    138.000
      0.215    120.000
      0.240    102.000
      0.250    101.000
      0.300    104.000
      0.330     89.000
      0.370     93.000
      0.410     86.000
      0.490     86.000

References:
1. G. I. Kanel', A. A. Razorenov, A. V. Utkin, K. Baumung, Experimental profiles
   of shock waves, Preprint of Scientific Association IVTAN of RAS (1996)