Copper M2, R0 =  8.930 g/cc

Target: 
  Sample density R0 = 8.93 g/cc, bulk sound velocity C0 = 3.96 km/s, longitudial sound velocity Cl = 4.6 km/s
  Sample thickness 3.9 mm (rod, batch II)
Loading: 
  Aluminum impactor 0.2 mm thick, impactor velocity 660 +/- 20 m/s
Experiment type: Laser interferometer (VISAR)

     t, mks     V, m/s

      0.000      0.000
      0.012      2.000
      0.040      6.000
      0.051     10.000
      0.062     23.000
      0.066     36.000
      0.078    145.000
      0.080    152.000
      0.081    162.000
      0.085    164.000
      0.095    161.000
      0.102    157.000
      0.110    150.000
      0.125    135.000
      0.150     89.000
      0.160     83.000
      0.170     79.000
      0.184     76.000
      0.250     68.000
      0.350     61.000
      0.450     56.000

References:
1. G. I. Kanel', A. A. Razorenov, A. V. Utkin, K. Baumung, Experimental profiles
   of shock waves, Preprint of Scientific Association IVTAN of RAS (1996)