Aluminum D16, R0 =  2.780 g/cc

Target: 
  Sample density R0 = 2.78 g/cc, bulk sound velocity C0 = 5.25 km/s, longitudial sound velocity Cl = 6.4 km/s
  Sample thickness 10 mm (rod)
  Copper baseplate 10 mm thick
Loading: 
  High explosive in contact with sample
Experiment type: Capacitor gauge

     t, mks     V, m/s

      0.000      0.000
      0.130     36.000
      0.220     40.000
      0.250     46.000
      0.400    548.000
      0.450    580.000
      0.530    588.000
      1.630    552.000
      2.110    555.000
      2.470    563.000
      3.080    544.000
      3.400    546.000
      3.780    558.000
      3.980    558.000

References:
1. G. I. Kanel', A. A. Razorenov, A. V. Utkin, K. Baumung, Experimental profiles
   of shock waves, Preprint of Scientific Association IVTAN of RAS (1996)