Aluminum D16, R0 =  2.780 g/cc

Target: 
  Sample density R0 = 2.78 g/cc, bulk sound velocity C0 = 5.25 km/s, longitudial sound velocity Cl = 6.4 km/s
  Sample thickness 10 mm (rod)
Loading: 
  Aluminum impactor 2 mm thick, impactor velocity 450 +/- 20 m/s
Experiment type: Capacitor gauge

     t, mks     V, m/s

      0.000      0.000
      0.110     34.000
      0.160     41.000
      0.210     72.000
      0.280    199.000
      0.360    409.000
      0.420    420.500
      0.480    421.000
      0.590    404.000
      0.750    368.000
      0.900    339.000
      0.960    333.000
      1.120    344.000
      1.490    335.000
      1.660    341.000
      1.780    340.000
      2.130    333.000

References:
1. G. I. Kanel', A. A. Razorenov, A. V. Utkin, K. Baumung, Experimental profiles
   of shock waves, Preprint of Scientific Association IVTAN of RAS (1996)