Aluminum D16, R0 =  2.780 g/cc

Target: 
  Sample density R0 = 2.78 g/cc, bulk sound velocity C0 = 5.25 km/s, longitudial sound velocity Cl = 6.4 km/s
  Sample thickness 10 mm (rod)
Loading: 
  Aluminum impactor 2 mm thick, impactor velocity 700 +/- 20 m/s
Experiment type: Capacitor gauge

     t, mks     V, m/s

      0.000      0.000
      0.090     35.000
      0.160     53.000
      0.180     59.000
      0.320    476.000
      0.390    484.000
      0.460    481.000
      0.550    470.000
      0.640    453.000
      0.750    421.000
      0.860    396.000
      0.950    397.000
      1.070    401.000
      1.200    396.000
      1.350    386.000
      1.430    388.000
      1.590    400.000
      1.720    401.000
      1.870    392.000
      1.960    391.000

References:
1. G. I. Kanel', A. A. Razorenov, A. V. Utkin, K. Baumung, Experimental profiles
   of shock waves, Preprint of Scientific Association IVTAN of RAS (1996)