Steel EP-836, R0 =  8.430 g/cc

Target: 
  Sample density R0 = 8.43 g/cc, bulk sound velocity C0 = 4.65 km/s, longitudial sound velocity Cl = 5.62 km/s
  Sample thickness 3.75 mm (rod)
Loading: 
  Aluminum impactor 0.4 mm thick, impactor velocity 720 +/- 20 m/s
Experiment type: Laser interferometer (VISAR)

     t, mks     V, m/s

      0.000      0.000
      0.015     14.000
      0.030     23.000
      0.040     36.000
      0.050     55.000
      0.100    199.000
      0.114    221.252
      0.130    226.000
      0.138    223.369
      0.144    216.138
      0.162    166.490
      0.170    144.000
      0.186    110.317
      0.200     89.000
      0.225     56.000
      0.240     40.000
      0.264     19.136
      0.290      8.000
      0.340      7.000

References:
1. G. I. Kanel', A. A. Razorenov, A. V. Utkin, K. Baumung, Experimental profiles
   of shock waves, Preprint of Scientific Association IVTAN of RAS (1996)