Steel EP-836, R0 =  8.430 g/cc

Target: 
  Sample density R0 = 7.76 g/cc, bulk sound velocity C0 = 4.65 km/s, longitudial sound velocity Cl = 5.89 km/s
  Sample thickness 11.5 mm (rod, batch II)
Loading: 
  Aluminum impactor 2 mm thick, impactor velocity 660 +/- 20 m/s
Experiment type: Laser interferometer (VISAR)

     t, mks     V, m/s

      0.000      0.000
      0.041     73.000
      0.157    109.000
      0.277    173.000
      0.337    247.000
      0.387    326.000
      0.427    336.000
      0.477    334.000
      0.517    326.000
      0.702    249.030
      0.950    173.000
      1.010    155.000
      1.126    132.205
      1.397    106.000
      1.897     85.000
      2.350     80.000

References:
1. G. I. Kanel', A. A. Razorenov, A. V. Utkin, K. Baumung, Experimental profiles
   of shock waves, Preprint of Scientific Association IVTAN of RAS (1996)