Magnesium Ma1, R0 =  1.750 g/cc

Target: 
  Sample density R0 = 1.75 g/cc, bulk sound velocity C0 = 4.5 km/s, longitudial sound velocity Cl = 5.61 km/s
  Sample thickness 4.9 mm (sheet)
Loading: 
  Aluminum impactor 0.2 mm thick, impactor velocity 660 +/- 20 m/s
Experiment type: Capacitor gauge

     t, mks     V, m/s

      0.000      0.000
      0.023     47.000
      0.078     49.000
      0.108     61.000
      0.139     87.000
      0.164    126.000
      0.185    171.000
      0.197    201.000
      0.205    235.000
      0.215    243.000
      0.229    242.416
      0.249    231.393
      0.278    209.000
      0.325    168.000
      0.360    138.801
      0.430     91.000
      0.468     79.630
      0.534     71.000
      0.655     64.374
      0.800     62.000
      0.950     62.000

References:
1. G. I. Kanel', A. A. Razorenov, A. V. Utkin, K. Baumung, Experimental profiles
   of shock waves, Preprint of Scientific Association IVTAN of RAS (1996)