Magnesium Ma1, R0 =  1.750 g/cc

Target: 
  Sample density R0 = 1.75 g/cc, bulk sound velocity C0 = 4.5 km/s, longitudial sound velocity Cl = 5.61 km/s
  Sample thickness 4.9 mm (sheet)
Loading: 
  Aluminum impactor 0.4 mm thick, impactor velocity 660 +/- 20 m/s
Experiment type: Capacitor gauge

     t, mks     V, m/s

      0.000      0.000
      0.012      8.000
      0.029     37.000
      0.082     50.000
      0.107     65.000
      0.142    172.487
      0.194    415.000
      0.216    465.000
      0.254    442.000
      0.276    424.000
      0.353    346.000
      0.400    293.651
      0.427    270.000
      0.496    287.654
      0.536    292.000
      0.589    280.000
      0.648    258.000
      0.771    262.000
      1.079    250.000
      1.450    250.000

References:
1. G. I. Kanel', A. A. Razorenov, A. V. Utkin, K. Baumung, Experimental profiles
   of shock waves, Preprint of Scientific Association IVTAN of RAS (1996)