Magnesium Ma1, R0 =  1.750 g/cc

Target: 
  Sample density R0 = 1.75 g/cc, bulk sound velocity C0 = 4.5 km/s, longitudial sound velocity Cl = 5.61 km/s
  Sample thickness 2 mm (sheet)
Loading: 
  Aluminum impactor 0.2 mm thick, impactor velocity 660 +/- 20 m/s
Experiment type: Capacitor gauge

     t, mks     V, m/s

      0.000      0.000
      0.014     11.000
      0.031     35.000
      0.095    400.000
      0.103    425.000
      0.124    397.000
      0.150    348.000
      0.181    289.000
      0.221    211.000
      0.270    253.000
      0.338    224.000
      0.378    240.000
      0.430    227.000
      0.500    235.000
      0.750    235.000

References:
1. G. I. Kanel', A. A. Razorenov, A. V. Utkin, K. Baumung, Experimental profiles
   of shock waves, Preprint of Scientific Association IVTAN of RAS (1996)