Steel 3, R0 =  7.850 g/cc

Target: 
  Sample density R0 = 7.85 g/cc, bulk sound velocity C0 = 4.65 km/s, longitudial sound velocity Cl = 5.97 km/s
  Sample thickness 5 mm (rod)
Loading: 
  Aluminum impactor 2 mm thick, impactor velocity 5300 +/- 150 m/s
Experiment type: Laser interferometer (VISAR)

     t, mks     V, m/s

      0.064      0.000
      0.120     10.000
      0.370     13.000
      0.375    160.000
      0.390   3220.000
      0.400   3327.000
      0.490   3237.000
      0.530   3178.000
      0.560   3208.000
      0.640   3185.000
      0.660   3195.000

References:
1. G. I. Kanel', A. A. Razorenov, A. V. Utkin, K. Baumung, Experimental profiles
   of shock waves, Preprint of Scientific Association IVTAN of RAS (1996)