Magnesium Mg95, R0 =  1.738 g/cc

Target: Magnesium Mg95, "original" cast magnesium
  Sample density R0 = 1.738 g/cc, bulk sound velocity C0 = 4.5 km/s, longitudial sound velocity Cl = 5.61 km/s
  Sample thickness 0.8 mm (bar)
Loading: 
  High-power ion beam
Experiment type: Laser interferometer (ORVIS)

     t, ns      V, m/s

      0.000      0.000
      1.745   3104.530
      3.114   3159.259
      4.995   3145.740
      6.745   3132.000
     15.245   2967.160
     16.245   2946.550
     17.595   2960.290
     18.995   2964.410
     19.745   2967.160
     21.495   2956.170
     23.495   2932.820
     25.745   2919.080
     28.595   2913.580
     31.495   2898.470
     37.245   2871.000
     46.495   2857.260
     55.495   2827.040
     64.995   2805.060
     75.495   2788.580

References:
1. G. I. Kanel\', A. A. Razorenov, A. V. Utkin, K. Baumung, Experimental profiles
   of shock waves, Preprint of Scientific Association IVTAN of RAS (1996)