Steel 45, R0 =  7.780 g/cc

Target: 
  Sample density R0 = 7.78 g/cc, bulk sound velocity C0 = 4.65 km/s, longitudial sound velocity Cl = 5.98 km/s
  Sample thickness 11.1 mm (rod)
Loading: 
  High explosive in contact with sample
Experiment type: Laser interferometer (VISAR)

     t, mks     V, m/s

      0.080      0.000
      0.085     28.000
      0.170     35.000
      0.300     55.000
      0.310     82.000
      0.395    331.000
      0.440    431.000
      0.500    434.000
      0.800    433.000
      1.000    430.000
      1.200    425.000
      2.040    370.000
      3.010    303.000
      3.830    228.000
      4.240    303.000
      4.400    331.000
      4.840    387.000

References:
1. G. I. Kanel', A. A. Razorenov, A. V. Utkin, K. Baumung, Experimental profiles
   of shock waves, Preprint of Scientific Association IVTAN of RAS (1996)