Molybdenum, R0 = 10.206 g/cc

Target: Molybdenum single crystal
  Sample density R0 = 10.21 g/cc, bulk sound velocity C0 = 5.14 km/s, longitudial sound velocity Cl = 6.44 km/s
  Sample thickness 0.275 mm (deformed 90-95%)
Loading: 
  Aluminum impactor 0.01 mm thick, impactor velocity 4100 +/- 150 m/s
  (in direction <100>)
Experiment type: Laser interferometer (ORVIS)

     t, ns      V, m/s

      0.000      0.000
      0.266   1070.000
      0.290   1080.000
      0.598   1103.420
      0.954   1101.070
      1.356   1091.450
      1.880   1046.150
      2.396    973.500
      2.879    886.110
      3.385    764.100
      3.741    661.110
      3.950    730.000
      4.200    790.000
      4.450    850.000
      4.909    950.000

References:
1. G. I. Kanel', A. A. Razorenov, A. V. Utkin, K. Baumung, Experimental profiles
   of shock waves, Preprint of Scientific Association IVTAN of RAS (1996)