Molybdenum, R0 = 10.206 g/cc

Target: 
  Sample density R0 = 10.21 g/cc, bulk sound velocity C0 = 5.14 km/s, longitudial sound velocity Cl = 6.44 km/s
  Sample thickness 5.9 mm (sintered rod)
  Aluminum baseplate 4.9 mm thick
Loading: 
  Aluminum impactor 2 mm thick, impactor velocity 660 +/- 20 m/s
Experiment type: Laser interferometer (VISAR)

     t, mks     V, m/s

      0.000      0.000
      0.040     38.820
      0.150     82.490
      0.220    117.600
      0.280    191.320
      0.304    237.160
      0.339    289.259
      0.360    298.790
      0.440    290.000
      0.700    249.230
      0.960    251.250
      1.140    241.650
      1.300    240.000

References:
1. G. I. Kanel', A. A. Razorenov, A. V. Utkin, K. Baumung, Experimental profiles
   of shock waves, Preprint of Scientific Association IVTAN of RAS (1996)