Molybdenum, R0 = 10.206 g/cc

Target: 
  Sample density R0 = 10.21 g/cc, bulk sound velocity C0 = 5.14 km/s, longitudial sound velocity Cl = 6.44 km/s
  Sample thickness 2.07 mm (sintered rod)
  Aluminum baseplate 2 mm thick
Loading: 
  Aluminum impactor 0.4 mm thick, impactor velocity 660 +/- 20 m/s
Experiment type: Laser interferometer (VISAR)

     t, mks     V, m/s

      0.000      0.000
      0.040     28.850
      0.080     95.140
      0.110    180.000
      0.120    188.290
      0.144    180.459
      0.230     99.750
      0.270    118.930
      0.340     98.390
      0.570     94.970

References:
1. G. I. Kanel', A. A. Razorenov, A. V. Utkin, K. Baumung, Experimental profiles
   of shock waves, Preprint of Scientific Association IVTAN of RAS (1996)