Molybdenum, R0 = 10.206 g/cc

Target: Molybdenum single crystal
  Sample density R0 = 10.21 g/cc, bulk sound velocity C0 = 5.14 km/s, longitudial sound velocity Cl = 6.44 km/s
  Sample thickness 1.37 mm 
  Aluminum baseplate 2 mm thick
Loading: 
  Aluminum impactor 0.4 mm thick, impactor velocity 660 +/- 20 m/s
  (in direction <110>)
Experiment type: Laser interferometer (VISAR)

     t, mks     V, m/s

      0.000      0.000
      0.020      3.000
      0.030      6.000
      0.039     12.860
      0.059     97.280
      0.076     64.780
      0.082     67.000
      0.095     74.000
      0.156    164.010
      0.304     81.650
      0.414     39.910
      0.673     88.400
      0.895     58.750

References:
1. G. I. Kanel', A. A. Razorenov, A. V. Utkin, K. Baumung, Experimental profiles
   of shock waves, Preprint of Scientific Association IVTAN of RAS (1996)