Lead, R0 = 11.346 g/cc

Target: 
  Sample density R0 = 11.35 g/cc, bulk sound velocity C0 = 2.03 km/s, longitudial sound velocity Cl = 2.25 km/s
  Sample thickness 3.6 mm (cast and pressed)
  Aluminum baseplate 4.1 mm thick
Loading: 
  Aluminum impactor 2 mm thick, impactor velocity 1900 +/- 70 m/s
Experiment type: Laser interferometer (VISAR)

     t, ns      V, m/s

     17.000      0.000
     17.000    199.000
     17.000   1205.000
     18.200   1288.860
     21.600   1310.000
     25.000   1313.000
     30.200   1313.350
     81.799   1301.429
    115.026   1291.857
    142.200   1285.250
    170.000   1293.000
    176.700   1294.230
    211.200   1287.820
    299.000   1284.510

References:
1. G. I. Kanel', A. A. Razorenov, A. V. Utkin, K. Baumung, Experimental profiles
   of shock waves, Preprint of Scientific Association IVTAN of RAS (1996)