Tin, R0 =  7.300 g/cc

Target: 
  Sample density R0 = 7.29 g/cc, bulk sound velocity C0 = 2.61 km/s, longitudial sound velocity Cl = 3.43 km/s
  Sample thickness 5 mm (cast and pressed)
  Aluminum baseplate 4.95 mm thick
Loading: 
  Aluminum impactor 1.8 mm thick, impactor velocity 2000 +/- 70 m/s
Experiment type: Laser interferometer (VISAR)

     t, mks     V, m/s

      0.023      0.000
      0.023     99.000
      0.023   1405.000
      0.029   1478.180
      0.033   1478.000
      0.085   1458.000
      0.106   1454.300
      0.115   1454.500
      0.150   1465.000
      0.158   1465.890
      0.170   1465.000
      0.250   1455.000
      0.299   1452.260
      0.428   1457.280
      0.599   1455.160

References:
1. G. I. Kanel', A. A. Razorenov, A. V. Utkin, K. Baumung, Experimental profiles
   of shock waves, Preprint of Scientific Association IVTAN of RAS (1996)