Paraffin, R0 =  0.917 g/cc

    m        U1       P1      dU12      P2    Rem  Ref
  1.019    2.570   15.400    2.660   54.600         1
  1.019    2.030   10.900    2.035   34.400         2
  1.019    2.140   11.800    1.580   29.900         3
  1.019    2.140   11.800    2.140   38.800         3

References:
1. L. V. Al'tshuler, A. P. Petrunin, Rentgenographic investigation of
   compressibility of light substances under obstacle impact of shock waves, Zh.
   Tekhn. Fiz. 31(6), 717-725 (1961) [in Russian]
2. L. V. Al'tshuler, M. N. Pavlovskii, Magnetoelectric method of definition of
   density behind front of colliding shock waves, Zh. Prikl. Mekh. Tekhn. Fiz. 2,
   110-114 (1971) [in Russian]
3. N. G. Kalashnikov, M. N. Pavlovskii, Investigation of shock compressibility of
   quartzite, paraffin and polytetrafluoroethylene with the help of manganin
   gauge, Zh. Prikl. Mekh. Tekhn. Fiz. 1, 181-183 (1975) [in Russian]

Denotions:
R0    - normal density of substance, g/cc
m     - porosity of sample
U1    - particle velocity on shock Hugoniot, km/s
P1    - pressure on shock Hugoniot, GPa
dU12  - jump of particle velocity on the front of reflected shock wave, km/s
P2    - pressure behind the second shock, GPa