Ceramic (BaTi3 - CaTi3), R0 =  5.540 g/cc

    m        U1       P1      dU12      P2    Rem  Ref
  1.000    0.085    2.960   -0.050    4.500         1
  1.000    0.085    2.960   -0.036    4.100         1
  1.000    0.087    3.020   -0.041    4.200         1
  1.000    0.088    3.040   -0.038    4.100         1
  1.000    0.088    3.040   -0.030    3.900         1
  1.000    0.088    3.060   -0.039    4.400         1
  1.000    0.089    3.080   -0.040    4.300         1
  1.000    0.089    3.110   -0.048    4.500         1
  1.000    0.107    3.700   -0.493   13.300         1
  1.000    0.108    3.700   -0.452   12.500         1
  1.000    0.108    3.800   -0.392    6.700         1
  1.000    0.110    4.000   -0.870   24.500         1

References:
1. M. van Thiel (Ed.), Compendium of shock wave data, (Livermore: Lawrence
   Livermore Laboratory Report UCRL-50108, 1977), 434-437

Denotions:
R0    - normal density of substance, g/cc
m     - porosity of sample
U1    - particle velocity on shock Hugoniot, km/s
P1    - pressure on shock Hugoniot, GPa
dU12  - jump of particle velocity on the front of reflected shock wave, km/s
P2    - pressure behind the second shock, GPa