Iron-chromium alloy, R0 =  7.773 g/cc

    m        U1       P1      dU12      P2    Rem  Ref
  1.000    0.384   15.500   -0.176   21.300         1
  1.002    0.329   13.100   -0.009   13.400         1
  1.002    0.337   13.400   -0.012   13.800         1
  1.006    0.393   15.700   -0.179   21.700         1
  1.017    0.499   20.700   -0.245   30.400         1
  1.017    0.499   20.700   -0.251   30.500         1
  1.020    0.572   23.800   -0.170   30.200         1
  1.021    0.536   22.300   -0.228   31.100         1

References:
1. M. van Thiel (Ed.), Compendium of shock wave data, (Livermore: Lawrence
   Livermore Laboratory Report UCRL-50108, 1977)

Denotions:
R0    - normal density of substance, g/cc
m     - porosity of sample
U1    - particle velocity on shock Hugoniot, km/s
P1    - pressure on shock Hugoniot, GPa
dU12  - jump of particle velocity on the front of reflected shock wave, km/s
P2    - pressure behind the second shock, GPa