Steel, 1020 alloy, R0 =  7.839 g/cc

    m        U1       P1      dU12      P2    Rem  Ref
  1.000    0.026    1.240   -0.316   13.710         1
  1.000    0.026    1.240   -0.196    9.050         1
  1.000    0.024    1.130   -0.146    6.980         1
  1.000    0.024    1.130   -0.166    7.740         1
  1.000    0.026    1.190   -0.244   10.950         1
  1.000    0.027    1.260   -0.290   12.860         1
  1.000    0.033    1.540   -0.277   12.920         1
  1.000    0.026    1.260   -0.219   10.010         1

References:
1. M. van Thiel (Ed.), Compendium of shock wave data, (Livermore: Lawrence
   Livermore Laboratory Report UCRL-50108, 1977), 182-191

Denotions:
R0    - normal density of substance, g/cc
m     - porosity of sample
U1    - particle velocity on shock Hugoniot, km/s
P1    - pressure on shock Hugoniot, GPa
dU12  - jump of particle velocity on the front of reflected shock wave, km/s
P2    - pressure behind the second shock, GPa