Steel, 1040 alloy, R0 =  7.834 g/cc

    m        U1       P1      dU12      P2    Rem  Ref
  1.000    0.029    1.380   -0.307   13.590         1
  1.000    0.033    1.500   -0.240   11.100         1
  1.000    0.029    1.380   -0.195    9.150         1
  1.002    0.025    1.120   -0.225   10.240         1

References:
1. M. van Thiel (Ed.), Compendium of shock wave data, (Livermore: Lawrence
   Livermore Laboratory Report UCRL-50108, 1977), 182-191

Denotions:
R0    - normal density of substance, g/cc
m     - porosity of sample
U1    - particle velocity on shock Hugoniot, km/s
P1    - pressure on shock Hugoniot, GPa
dU12  - jump of particle velocity on the front of reflected shock wave, km/s
P2    - pressure behind the second shock, GPa